TROUBLESHOOTING / FLOW & JETTING
Flow marks and jetting are flow-history evidence.
Flow marks appear as wavy, matte or orientation lines on the surface. Jetting is a snake-like or spraying defect that can occur when the melt enters the cavity as a free jet instead of a stable flow front. Gate design, fill speed, temperature, venting and material behavior all matter.
ABERY engineering note
Updated November 20, 2026
Do not increase injection speed automatically. Faster fill can worsen jetting or shear in some gates and improve it in others. The gate and flow pattern must be understood.
QUICK ANSWER
Record the defect location, gate type, fill time, injection speed, melt and mold temperature, material lot, part thickness and venting condition. Compare a short shot with the full part and review the gate and flow front. Correct the dominant flow source and validate appearance, dimensions and strength across cavities.
1. Separate flow marks from jetting.
A flow mark follows the advancing front or a change in cooling and orientation. Jetting usually radiates from the gate and may show a folded or snake-like path.
The pattern should be photographed before changing settings. A defect that begins at the gate points to gate and injection conditions; a defect at a rib or last-fill area may point to flow, cooling or venting.
| Flow mark | Wavy, matte or orientation line. |
|---|---|
| Jetting | Snake or spray pattern from gate. |
| Gate area | Shear, freeze or free jet. |
| Last fill | Gas trap or pressure loss. |
| Rib/transition | Flow hesitation or cooling. |
| Weld line | Flow-front merge and strength. |
2. Review gate type and entry.
A gate that enters a thick cavity without a controlled transition can create a free jet. Gate size, land, angle and location should support a stable flow front.
A larger gate or a different gate type may reduce jetting but affect cosmetics, degating and cycle. Compare the options with the part appearance and material.
- Gate type and size.
- Gate land and entry angle.
- Gate location relative to wall.
- Runner and pressure.
- Degating and cosmetic mark.
- Material shear behavior.
3. Control fill speed and heat history.
Injection speed changes shear, fill time, cooling and orientation. A speed that is too low can allow the front to freeze; a speed that is too high can create jetting, burn or stress.
Melt and mold temperature should be reviewed with the material recommendation and actual part quality. A temperature change can reduce viscosity but also increase degradation risk.
| Injection speed | Fill stability and shear. |
|---|---|
| Melt temp | Viscosity and heat history. |
| Mold temp | Cooling and surface. |
| Packing | Stress and dimension. |
| Material | Viscosity and additive. |
| Vent | Gas release at the front. |
4. Improve venting and flow transitions.
Trapped gas can create burn, short shots and surface defects near the last-fill area. A vent path should follow the flow front and be accessible for cleaning.
Abrupt wall changes and poorly placed ribs can make the flow hesitate. The tool and part design may need a transition change rather than a process-only correction.
- Vent location and depth.
- Last-fill area.
- Flow leaders and thickness transitions.
- Ribs and bosses.
- Weld-line location.
- Maintenance access.
5. Validate the corrected surface.
Compare the corrected part with the approved appearance boundary at the same lighting and viewing distance. Check all cavities and the first parts after startup.
If the defect is cosmetic, keep a boundary sample. If it affects strength or sealing, include the relevant functional test.
- Flow and jetting pattern.
- Appearance boundary.
- Cavity and shot identification.
- Process settings.
- Functional or strength check.
- Revalidation trigger.
Questions buyers ask before approving this scope.
What is the difference between a flow mark and jetting?
Can higher injection speed remove flow marks?
Are flow marks only cosmetic?
What information should be sent for review?
Need a project-specific answer?
Send the part, material, volume and stage. We will identify what can be confirmed before quotation or tooling.
Send the projectContinue the engineering review.
Keep the scope comparable.
The linked guides are written to support a project-specific supplier and tooling review.
PROJECT INTAKE / FLOW DEFECT
Send the gate, fill pattern and surface standard.
We will help separate gate, speed, temperature, venting and material causes before the next process change.
Tell us where the project is now.
Send the files and context you have. Missing information can be confirmed during review.
Business inquiries only. For large files, include a secure Google Drive, Dropbox, OneDrive or WeTransfer link, or email tonney@a-mold.com after submitting.